C3604 (C36000) Brass for Turned Parts

MaterialsCNC machiningMaterialsNov 9, 2026

C3604 (free-cutting brass, similar to C36000) is a free-cutting brass bar stock made by adding 1.8 to 3.7% lead to brass, an alloy of copper and zinc, to improve machinability; when a turned-part drawing lists brass in the material field, it is mostly this material. The lead in the microstructure breaks chips short, so it cuts easily, and small rotational parts such as fittings, nozzles, pins, and inserts are often made from it. Choose the material based on whether the part is machined and on the type of water the part contacts: specify lead-free brass for parts that contact drinking water, and DZR brass for parts that contact seawater or hot water.

Types and Designation Codes

Brass is an alloy of copper and zinc, and even among brasses the composition differs between bar and sheet, so they are distinguished by designation. Many shops in Korea use JIS designations (C plus 4 digits) as they are.

DesignationCategoryMain compositionMain use
C3604Free-cutting brass bar (JIS H 3250)Cu 57.0 to 61.0%, Pb 1.8 to 3.7%, Zn balanceTurned machined parts
C2801Brass sheet (JIS H 3100)Cu 59.0 to 62.0%, Pb 0.10% max, Zn balanceStamping, bending, decorative plate
C6804, etc.Lead-free free-cutting brass (bismuth type, JIS H 3250)Bi 1.8 to 3.7% instead of lead, Pb 0.10% maxMachined parts subject to lead regulation
C6931Lead-free free-cutting brass (silicon type, JIS H 3250)Cu 74 to 79%, Si 2.6 to 3.4%Plumbing parts, machined parts needing strength

C2801 is a sheet grade with good bending and stamping formability, but when machined its chips run long, so specify C3604 by default for parts turned from bar stock.

Characteristics

Lead barely mixes with copper and zinc and is dispersed as fine particles in the microstructure; during cutting these particles become the starting points where chips break and also act as a lubricant between the tool and the chip. As a result, chips break and fall away short, tool wear stays low even at higher feed rates, and the machined surface is clean. The US alloy C36000, which has a similar composition, is used as the reference value (100) of the copper alloy machinability index.

In continuous automatic lathe machining, chip handling largely determines productivity, so the higher the quantity, the greater the advantage of free-cutting brass. The features of the turning process are covered in the CNC Turning Guide, and how to judge geometries that also need milling is covered in CNC Milling vs. Turning.

Applications

  • Fittings, nozzles, valve parts: rotational parts with many threads and holes, with adequate corrosion resistance in air and fresh water
  • Electrical terminals and connector pins: higher electrical conductivity than steel or SUS, and easy to solder and plate
  • Insert nuts and spacers: inserts for plastic parts are often made of brass. A comparison of thread reinforcement methods is covered in Helicoil vs. Insert Nut
  • Decorative items, nameplates, handles: polishing gives a gold luster, and it is also used as a base material for nickel and chrome plating

Comparison with Aluminum and SUS

ItemC3604AL6061SUS304
MachinabilityVery goodGoodPoor (difficult-to-machine)
Density (g/cm³)About 8.5About 2.7About 7.9
Electrical conductivity (%IACS)About 26About 40About 2 to 3
Corrosion resistanceGood in air and fresh water; watch for dezincificationGood (improved with anodizing)Excellent
Material costVaries widely with the copper market price. For the same volume, brass weighs more than 3 times as much as aluminum, so material cost tends to be a burden

Brass suits parts that need conductivity and appearance in a large quantity of small rotational parts; aluminum suits cases where weight matters, and SUS suits cases where corrosion resistance and strength come first.

Lead Regulation and Dezincification

RoHS: EU RoHS allows copper alloys with up to 4% lead under exemption 6(c), so C3604, with a maximum of 3.7% lead, currently falls within the exemption. However, the EU sets a time limit on this exemption and renews it (most recently extended to June 30, 2027), so for parts in exported electronics, first check the customer's lead standard.

Drinking water: Lead limits for parts that contact drinking water are far stricter, and in the US only a weighted average lead content of 0.25% or less on the wetted surface is recognized as lead-free. Specify lead-free brass such as C6931 for such parts, and for plumbing parts in Korea also check whether hygiene and safety standard certification applies.

Dezincification: When brass with high zinc content contacts salty or stagnant water for a long time, only the zinc leaches out and a porous copper structure remains. This corrosion leaves the outward appearance unchanged while strength drops, easily leading to thread failure or leaks, so for parts that contact seawater or hot water, consider dezincification-resistant (DZR) brass, bronze, or SUS.

Surface Finish

Left as is, brass darkens by oxidation, so a clear coating is commonly used to keep its appearance, nickel plating for wear resistance and appearance, and chrome plating over nickel for decoration, and tin, silver, or gold plating is also used for electrical terminals. The characteristics of each plating type are covered in Plating Types for Steel Parts, and many of them also apply to brass, but anodizing, which is a treatment for aluminum, cannot be applied to brass.

Drawing and Purchase Order Notation

  • Material: write "C3604", or include the stock form as "C3604BD". Writing the designation is what distinguishes it from sheet brass
  • Lead restriction: where applicable, write "lead-free brass" together with the applicable regulation and limit value. For the US drinking water standard, write "weighted average Pb 0.25% max on wetted surface"
  • Surface finish: write the type and thickness, such as "electroless nickel plating 5μm", and if plating affects press fits or threads, state whether the dimension is before or after plating
  • Mill sheet: for parts subject to lead regulation, write the submission of a composition certificate as a requirement

Frequently Asked Questions

Can C3604 also be milled?

Yes. The advantage of short, broken chips is the same in milling, but commercially available stock is mostly bar, so for a large block shape, first check whether stock in that size is available.

Can brass parts be welded?

Soldering and brazing are possible. However, with arc welding of C3604, zinc tends to vaporize and the lead can cause cracking, so join by soldering or brazing and generally avoid arc welding.

Do machining conditions change if you switch to lead-free brass?

They can; bismuth-type and silicon-type lead-free brasses are known to have somewhat lower machinability than C3604. For parts being switched to lead-free brass, check machining time and the quote separately on a lead-free brass basis.

Summary

For small turned parts, C3604 is the default brass; write "C3604" in the drawing's material field to distinguish it from sheet-grade C2801, and specify lead-free brass for parts that contact drinking water and DZR brass, bronze, or SUS for parts that contact seawater or hot water. C3604 currently falls within the RoHS exemption, but the exemption has a time limit, so for exported electronics check the customer's standard.

To request a quote for C3604 parts, upload a STEP file to MakeIT.

Have a part to machine?